| Magnesia ceramic (Dense Magnesia) | ||||
| Chemical composition: MgO | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 3.4 *10³ | kg/m³ | 212.2 | lb/ft³ | 
|---|---|---|---|---|
| Modulus of elasticity | 250 | GPa | 36300 | ksi | 
| Flexural strength | 165 | MPa | 23900 | psi | 
| Thermal expansion (20 ºC) | 13.5*10-6 | ºCˉ¹ | 7.5*10-6 | in/(in* ºF) | 
| Thermal conductivity | 9 | W/(m*K) | 62.4 | BTU*in/(hr*ft²*ºF) | 
| Specific heat capacity | 880 | J/(kg*K) | 0.21 | BTU/(lb*ºF) | 
| Dielectric constant (1MHz) | 10 | - | 10 | - | 