| Spinodal Bronze ToughMet2 CX | ||||
| Chemical composition: Ni=9.0%, Sn=6.0%, Cu=balance | ||||
| Property | Value in metric unit | Value in US unit | ||
| Density | 8.91*10³ | kg/m³ | 556 | lb/ft³ |
|---|---|---|---|---|
| Modulus of elasticity | 117 | GPa | 17000 | ksi |
| Thermal expansion (20 ºC) | 16.7*10-6 | ºCˉ¹ | 9.3*10-6 | in/(in* ºF) |
| Specific heat capacity | 381 | J/(kg*K) | 0.091 | BTU/(lb*ºF) |
| Thermal conductivity | 64.9 | W/(m*K) | 450 | BTU*in/(hr*ft²*ºF) |
| Thermal diffusivity | 1.68*10-5 | W/(m*K) | 0.026 | in²/s |
| Tensile strength (cast and spinodally hardened) | 743 | MPa | 108000 | psi |
| Yield strength (cast and spinodally hardened) | 655 | MPa | 95000 | psi |
| Elongation (cast and spinodally hardened) | 7.5 | % | 7.5 | % |
| Hardness (cast and spinodally hardened) | 28 | RC | 28 | RC |